公司承诺 |
|
|
|
|
|
钢材知识 |
|
|
|
准
|
牌号
|
抗拉强度(MPa)
|
屈服强度(MPa)
|
伸长率(%)
|
冲击功(J)
|
硬度
|
|
GB3087
|
10
|
335~475
|
≥195
|
≥24
|
|
/
|
|
20
|
410~550
|
≥245
|
≥20
|
|
/
|
|
GB5310
|
20G
|
410~550
|
≥245
|
≥24
|
≥35
|
/
|
|
20MnG
|
≥415
|
≥240
|
≥22
|
≥35
|
/
|
|
25MnG
|
≥485
|
≥275
|
≥20
|
≥35
|
/
|
|
15CrMoG
|
440~640
|
≥235
|
≥21
|
≥35
|
/
|
|
12Cr2MoG
|
450~600
|
≥280
|
≥20
|
≥35
|
/
|
|
12Cr1MoVG
|
470~640
|
≥255
|
≥21
|
≥35
|
/
|
|
10Cr9Mo1VNb
|
≥585
|
≥415
|
≥20
|
≥35
|
/
|
|
ASME SA106
|
SA106B
|
≥415
|
≥240
|
≥22
|
≥35
|
/
|
|
SA106C
|
≥485
|
≥275
|
≥20
|
≥35
|
/
|
|
ASME SA333
|
SA333Ⅰ级
|
≥380
|
≥205
|
≥28
|
-45℃
≥18
|
/
|
|
SA333Ⅵ级
|
≥415
|
≥240
|
≥22
|
-45℃
≥18
|
/
|
|
ASME SA335
|
SA335 P11
|
≥415
|
≥205
|
≥22
|
≥35
|
≤163HB
|
|
SA335 P12
|
≥415
|
≥220
|
≥22
|
≥35
|
≤163HB
|
|
SA335 P22
|
≥415
|
≥205
|
≥22
|
≥35
|
≤163HB
|
|
SA335 P5
|
≥415
|
≥205
|
≥22
|
≥35
|
≤187HB
|
|
SA335 P91
|
585~760
|
≥415
|
≥20
|
≥35
|
≤250HB
|
|
SA335 P92
|
≥620
|
≥440
|
≥20
|
≥35
|
250HB
|
|
DIN17175
|
ST45.8/Ⅲ
|
410~530
|
≥255
|
≥21
|
≥27(DVM)
|
/
|
|
15Mo3
|
450~600
|
≥270
|
≥22
|
≥34(DVM)
|
/
|
|
13CrMo44
|
440~590
|
≥290
|
≥22
|
≥34(DVM)
|
/
|
|
10CrMo910
|
480~630
|
≥280
|
≥20
|
≥34(DVM)
|
/
|
|
EN10216-2
|
15NiCuMoNb5-6-4 (WB36)
|
610~780
|
≥440
|
≥19
|
≥40
|
/
|
|
|
|
|
钢管种类
|
外径(D)
|
壁厚(S)
|
|
冷拔管
|
钢管外径(mm)
|
允许偏差(mm)
|
钢管壁厚(mm)
|
允许偏差(mm)
|
|
>114~159
|
±0.8%
|
≤30
|
±10%
|
|
>159~219
|
±1.0%
|
|
热轧管
|
>219~457
|
±1.0%
|
≤20
|
-10%+12.5%
|
|
>20~40
|
-10%,+10%
|
|
>457~1066
|
±0.9%
|
>40~70
|
-7%,+9%
|
|
>70~120
|
-6%,+8%
|
|
下一页:钢制压力容器焊接通用工艺目录[技术文章]
|
|
|